Jun 27, 2025 Leave a message

How to Choose the Specifications and Thickness of 1050 aluminium Coil

Why 1050 Coil Is the Starting Point for Thin Gauge Work

1050 is a commercially pure wrought aluminium grade with a minimum aluminium content of 99.50 percent, as listed in ASTM B209, and the closely related 1050A is defined in EN 573-3. Because there is no deliberate alloying addition, the coil keeps the two characteristics that matter most at thin gauge: high electrical and thermal conductivity, and a soft, highly formable structure in the annealed O temper. Conductivity in the O temper is typically around 61 percent IACS, which is why the grade is common in transformer windings, busbar covers and heat transfer components.

The material reaches the customer as cold rolled coil in O, H14, H18, H22 or H24 temper. Each temper corresponds to a different amount of cold reduction after annealing, and that reduction fixes the strength level and the tightest bend radius the strip can accept on a press brake, roll former or slitting line.

Thickness Ranges: Match the Gauge to the Forming Operation

Cold rolled 1050 coil is normally produced from 0.2 mm to 6.0 mm, and most tonnage sits between 0.3 mm and 3.0 mm. The sensible starting point is not the drawing tolerance but the forming step the strip has to survive:

0.2 to 0.5 mm: closures, lids, fin stock, cable wrap and flexible packaging, where the strip is curled on a very tight radius.

0.5 to 1.2 mm: insulation jacketing, duct wrap, nameplates and light windings; O temper is preferred for tight wrapping.

1.2 to 2.0 mm: deep drawn cookware, plate blanks, heat shields and formed covers, in O or H14 temper depending on draw depth.

2.0 to 3.5 mm: tank and vessel liners, sign substrates and general fabrication, usually in H14 or H24.

3.5 to 6.0 mm: covers, road sign blanks and machined parts, where stiffness matters more than formability.

A useful rule of thumb: every step up in temper hardness reduces the minimum bend radius the coil tolerates before cracking, so specify the softest temper that still meets the strength requirement of the finished part.

Dimensions and Tolerances to Write Into the Purchase Order

Width is limited by the rolling and slitting line. Common mills supply 1050 coil up to about 1500 mm, and wide mills reach 2650 mm. Inner diameter is normally 405 mm, 505 mm or 508 mm; outer diameter usually falls between 900 mm and 1700 mm; coil weight generally ranges from 1 t to 6 t. Heavier coils lower the handling cost per tonne but demand a decoiler that can carry them.

Thickness tolerance is controlled by ASTM B209 for American orders, EN 485-4 for European orders and GB/T 3880.3 for Chinese orders. At thin gauge the tolerance is expressed as a plus and minus band around nominal thickness, and the band tightens as the strip gets thinner. Width tolerance on slit coil is usually a minus-only band, camber is quoted in millimetres per metre of length, and flatness is quoted as maximum wave height over a stated length. If the strip feeds an automated press, name the tolerance class explicitly, because a nominal-gauge call-out leaves the mill free to ship the full standard band.

Temper and the Mechanical Properties Behind It

The table below gives typical bands for cold rolled 1050 coil; the mill certificate remains the reference for a specific heat.

Property 1050 O 1050 H14 1050 H18
Typical tensile strength 60 to 95 MPa 95 to 130 MPa 125 MPa and above
Typical 0.2 percent proof stress 15 MPa and above 70 MPa and above 110 MPa and above
Elongation at thin gauge 25 percent and above 4 percent and above 2 percent and above
Formability Excellent Good Limited
Bend radius trend Tightest Moderate Widest

The chemistry is narrow by design. ASTM B209 limits silicon plus iron to 0.45 percent maximum, copper to 0.05 percent, manganese to 0.05 percent, magnesium to 0.05 percent, zinc to 0.05 percent and titanium to 0.03 percent. EN 573-3 places 1050A at silicon 0.25 percent and iron 0.40 percent maximum. These limits protect conductivity, and they also mean that scrap with copper or magnesium contamination cannot be charged freely into the melt.

Ordering Checklist and Incoming Verification

Quote grade, temper, thickness and tolerance class separately. A request for 1050 coil alone is not a specification.

Quote width, inner diameter, outer diameter range, coil weight and eye to sky orientation.

State the surface requirement: mill finish, coil coated, PVC film laminated or paper interleaved.

Request a mill test certificate covering chemistry and mechanical properties for every coil.

On receipt, check thickness at several points across the width with a calibrated micrometer, compare camber against a straight edge over the full coil length, and match the temper mark on the coil tag to the certificate.

Keeping the three decisions separate, gauge for forming, temper for strength and tolerance class for the feeding equipment, removes most of the disputes that arise on thin aluminium coil orders.

Frequently Asked Questions

Q: Is 1050 the same as 1050A?
They are close equivalents. ASTM B209 lists 1050 with silicon plus iron at 0.45 percent maximum, while EN 573-3 limits 1050A to silicon 0.25 percent and iron 0.40 percent. Both are commercially pure aluminium with at least 99.50 percent aluminium.

Q: Which temper should I choose for a part that is bent after coating?
Use O or H22 for tight bends, because coil coated strip usually bends more easily in the softer tempers. If the part also carries load, step up to H14 and increase the bend radius rather than risking cracking at the coating line.

Q: How thick can 1050 coil be supplied?
Cold rolled production normally runs from 0.2 mm to 6.0 mm. Above that range the material is usually supplied as plate rather than coil, and the temper range narrows because heavy reduction is limited by mill torque.

Q: Can 1050 coil be welded?
Yes. The grade is readily welded by TIG or MIG processes with 1100 series filler, and it also joins well by resistance spot welding. Because the alloy is soft, thin sections need fixtures to control distortion.

Q: Why does 1050 have lower strength than 3003?
1050 contains almost no manganese, while 3003 carries about 1.0 to 1.5 percent manganese, which raises strength. When strength is the governing requirement, 3003 or 5052 is the better selection, at a higher price per tonne.

Q: What should be checked first when a coil arrives?
Check the coil tag against the mill certificate, then verify thickness across the width and camber over the coiled length. Surface defects such as dents or edge damage are best recorded before the coil is loaded onto the decoiler.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry