Aluminum-Alloy-3003-H14-Sheet-Aluminum-3003-H14-Plate.pdf
What is Alloy 3003 H14?
3003 aluminium alloy is a commercially pure aluminium with high mechanical qualities and is frequently used in industries. It is a medium-strength alloy with excellent resistance to air corrosion. The alloy has superior mechanical qualities when compared to 1000 series alloys and is 20% stronger than 1100.
H14: Strain-hardened, 1/2 hard.
Chemical Composition of Aluminum Alloy 3003
Chemical Composition (wt%) limits as specified in ASTM B209 and ASME SB209*
| Element | 3003 |
| Silicon | 0.6 |
| Iron | 0.7 |
| Copper | 0.05-0.20 |
| Manganese | 1.0-1.5 |
| Zinc | 0.10 |
| Aluminum | balance |
| Other Elements (each) | 0.05 |
| Other Elements (total) | 0.15 |
Mechanical Properties (H14 Temper):
| Property | Value |
|---|---|
| Tensile Strength | 22 – 29 ksi (152 – 200 MPa) |
| Yield Strength | 17 ksi (117 MPa) |
| Elongation | 5%–10% |
| Brinell Hardness | 40 HB |
Available Plate Sizes:
| Thickness (mm) | Width (mm) | Length (mm) |
|---|---|---|
| 0.5 mm – 6 mm | 500 mm – 2000mm | 1000 mm – 6000mm |
Alloy 3003 Standards & Specifications:
| Standard | Specification |
|---|---|
| ASTM | ASTM B209 |
| ASME | ASME SB209 |
| EN | EN 573-3, EN 485-2 |
| ISO | ISO 6361 |
Applications of 3003 H14 Aluminum Plate:
Roofing and cladding offer excellent weather resistance.
Food and beverage industry-Used for storage tanks and packaging.
Marine and automotive body panels are corrosion-resistant.
HVAC and insulation are used in ducting and as thermal barriers.
Chemical and pharmaceutical equipment-non-reactive and long-lasting.
Why Choose Our 3003 H14 Aluminum Plates?
High Corrosion Resistance – Ideal for outdoor & marine environments.
Excellent Workability-Easy to bend, weld, and machine.
Lightweight & Durable-Strong yet easy to handle.

What is the difference between 3003 H14 and 5052?
3003 H14 has an ultimate tensile strength range of 20–26 KSI, a yield of 21, an elongation of 8.3%, and a Brinell hardness of 40, while 5052 H32 has an ultimate tensile strength range of 31–38 KSI, a yield of 28, an elongation of 12%, and a Brinell hardness of 60.
Can you weld 3003 aluminum to 6061?
3003 aluminum is easily welded using traditional procedures. Filler rods are commonly made of aluminum 1100. When welding 3003 to other aluminum alloys such as 5052, 6061, or 6062, use a 4043 aluminum filler rod.
Advantages of 3003 Aluminum Sheet
1. Excellent rust-proof property.
2. Excellent plasticity, corrosion resistance, weldability, and conductivity.
3. Better strength than 1100 aluminum alloy.
4. Ideal choice for a power battery shell because of impact resistance; it is not easy to break or leak.
3003 Aluminum Plate/Sheet Mechanical Properties
|
Material |
Condition |
Tensile Strength (KSI) |
Yield Strength (KSI min) |
Elongation % |
Min 90° Cold Bend Radius for 0.064" Thick |
|
3003-0 sheet 0.064" thick |
3003-0 |
14-19 |
5 |
25 |
O |
|
3003-H12 sheet 0.064" thick |
3003-H12 |
17-23 |
12 |
6 |
O |
|
3003-H14 sheet 0.064" thick |
3003-H14 |
20-26 |
17 |
5 |
O |
|
3003-H16 sheet 0.064" thick |
3003-H16 |
24-30 |
21 |
4 |
1/2 - 1 1/2 T |
|
3003-sheet 0.064" thick |
3003-H18 |
27 min |
24 |
4 |
1 1/2 -3T |