5083-H116 is an aluminum alloy (5083) with a specific temper (H116), which is treated to enhance its corrosion resistance, classifying it as "marine-grade" aluminum. While there is no direct equivalent material, the closest match in terms of alloy composition and corrosion resistance is 5083-H321, which also offers similar properties with more stability, especially after painting. Other alloys from the 5xxx series, such as 5005, 5052, and 5383, may also be considered depending on the specific mechanical needs of the application.
Closest Equivalents
5083-H321: This is the most common alternative. While both alloys are marine-grade 5083 aluminum, H321 typically provides slightly higher hardness and stability, particularly after painting.
5083-H22: Shares the same alloy composition as 5083-H116 but differs in mechanical properties due to its processing.
5086-H116: Another marine-grade alloy chemically similar to 5083, offering comparable corrosion resistance.
How They Differ
Alloy vs. Temper: 5083 is the aluminum alloy, while H116 is the temper, indicating specific heat and strain treatments to achieve desired properties, such as enhanced corrosion resistance.
Properties: H116 is specifically processed for high corrosion resistance, making it ideal for marine applications. The H321 temper, while offering similar corrosion resistance, often delivers more stable performance, particularly in applications requiring post-painting.
Other 5xxx Series Alloys: Alloys like 5005 and 5052 have different chemical and mechanical properties and may be suitable alternatives when slightly different strength or corrosion resistance requirements exist.

Subcategory: 5000 Series Aluminum Alloy; Aluminum Alloy; Metal; Nonferrous Metal
Close Analogs:
Aluminum 5083-H321
UNS A95083
ISO AlMg4.5Mn
Aluminum 5083-H116
Aluminum 5083-H321
AA 5083-H116
Composition Notes:
The aluminum content is calculated as the remainder. Composition information provided by the Aluminum Association is not intended for design purposes.
| Component | Wt. % |
|---|---|
| Al | 92.4 - 95.6 |
| Cr | 0.05 - 0.25 |
| Cu | Max 0.1 |
| Fe | Max 0.4 |
| Mg | 4 - 4.9 |
| Mn | 0.4 - 1 |
| Si | Max 0.4 |
| Ti | Max 0.15 |
| Zn | Max 0.25 |
| Other, each | Max 0.05 |
| Other, total | Max 0.15 |
Material Notes:
Data points marked with AA are provided by the Aluminum Association and are not for design.
Physical Properties
| Property | Metric | English | Comments |
|---|---|---|---|
| Density | 2.66 g/cc | 0.0961 lb/in³ | AA; Typical |
Mechanical Properties
| Property | Value | Comments |
|---|---|---|
| Hardness, Brinell | 85 | 500 kg load with 10 mm ball. Calculated value. |
| Hardness, Knoop | 109 | Converted from Brinell Hardness Value |
| Hardness, Rockwell A | 36.5 | Converted from Brinell Hardness Value |
| Hardness, Rockwell B | 53 | Converted from Brinell Hardness Value |
| Hardness, Vickers | 96 | Converted from Brinell Hardness Value |
| Ultimate Tensile Strength | 317 MPa | 46,000 psi; AA; Typical |
| Tensile Yield Strength | 228 MPa | 33,000 psi; AA; Typical |
| Elongation at Break | 16% | 16%; AA; Typical (1/2 in. diameter) |
| Modulus of Elasticity | 70.3 GPa | 10,200 ksi; In Tension |
| Modulus of Elasticity | 71 GPa | 10,300 ksi; AA; Typical; Average of tension/compression |
| Compressive Modulus | 71.7 GPa | 10,400 ksi |
| Poisson's Ratio | 0.33 | Estimated from trends in similar Al alloys |
| Fatigue Strength | 159 MPa | 23,000 psi; 500,000,000 cycles reversed stress; RR Moore machine/specimen |
| Fracture Toughness | 43 MPa-m½ | 39.1 ksi-in½; KIC; TL orientation |
| Machinability | 30% | 0-100 Scale of Aluminum Alloys |
| Shear Modulus | 26.4 GPa | 3,830 ksi |
| Shear Strength | 190 MPa | 27,600 psi; Calculated value |
Electrical Properties
| Property | Metric | English | Comments |
|---|---|---|---|
| Electrical Resistivity | 5.9e-006 ohm-cm | 5.9e-006 ohm-cm |
Thermal Properties
| Property | Metric | English | Comments |
|---|---|---|---|
| CTE, linear at 68°F | 23.8 µm/m-°C | 13.2 µin/in-°F | AA; Typical; Average over 68-212°F range |
| CTE, linear at 250°C | 26 µm/m-°C | 14.4 µin/in-°F | Average over the range 20-300°C |
| Specific Heat Capacity | 0.9 J/g-°C | 0.215 BTU/lb-°F | |
| Thermal Conductivity | 117 W/m·K | 812 BTU-in/hr-ft²-°F | |
| Melting Point | 591 - 638 °C | 1095 - 1180 °F | AA; Typical range based on typical composition for wrought products 1/4 inch thickness or greater |
| Solidus | 591 °C | 1095°F | AA; Typical |
| Liquidus | 638 °C | 1180°F | AA; Typical |
Processing Properties
| Property | Metric | English | Comments |
|---|---|---|---|
| Annealing Temperature | 413 °C | 775 °F | Holding at temperature not required |
| Hot-Working Temperature | 316 - 482 °C | 600 - 900 °F |